Sillimanit and mullit fire-resistant materials
|
Fire-resistant materials made of mullit and sillimanit are fire-resistant, have thermostability, stability to corrosion and erosion of glass mass, i.e. they have very low pollution of glass mass, they are the most widely used kinds of fire-resistant materials for the device of a feeder, glass-blowing machines, making glass pipes in domestic and foreign glass manufactures. The presented nomenclature of fire-resistant products of this kind is those: a brick of the channel of a feeder, lowering tray, the core, a ring sleeve, a mixer, a needle, a tube of a feeder, foam-blocking bar, slide valve of furnaces, blocks of torches, a grid-iron brick, a platband, a brick of thermal furnaces and other products (more than 100 kinds) of the various sizes.
|
Chemical compound and physical parameters
| Parameters | Designation | The Product |
| Cast-sillimanit brick | Cast corundum-mullit brick | Sillimanit brick | Sintered mullit brick | Smelted mullit brick | Sintered corundum-mullit brick |
| CS | CCM | SA | SB | SM65 | SM70 | SM75 | SM80 | FM | SCM |
| Al2O3 ≥ | % | 58 | 80 | 58 | 60 | 64 | 68 | 74 | 78 | 72 | 80 |
| F2O3 ≤ | % | 0.8 | 0.5 | 0.8 | 1.0 | 1.2 | 1.2 | 0.8 | 0.8 | 0.5 | 0.5 |
| Fire resistance ≥ | °С | 1790 | 1810 | 1790 | 1790 | 1790 | 1790 | 1790 | 1810 | 1810 | 1830 |
| Porosity ≤ | % | 26 | 22 | 22 | 18 | 18 | 20 | 18 | 18 | 18 | 18 |
| Poured density | g/cm3 | 2.2 | 2.65 | 2.35 | 2.5 | 2.5 | 2.5 | 2.60 | 2.70 | 2.65 | 2.8 |
| Limit of strength at compression at low temperatures ≥ | MPa | 50 | 60 | 50 | 70 | 55 | 60 | 65 | 70 | 70 | 70 |
| Fire resistance under loading ≥ | °С | 1450 | 1650 | 1550 | 1600 | 1560 | 1580 | 1650 | 1700 | 1700 | 1700 |
| Linear change at repeated heating | 1400°Сх2h | % | +0.1~ -0.3 | | +0.1~ -0.1 | | | | | | | |
1500°Сх2h | % | | +0.1~ -0.2 | | +0.1~ -0.2 | +0.1~ -0.4 | +0.1~ -0.3 | +0.1~ -0.2 | +0.1~ -0.2 | +0.1~ -0.1 | +0.1~ -0.1 |
|
|
|